Causes and solutions of top whiteness in injection molding products

Release time:2021-08-16

When the plastic parts of injection products are ejected from the mold, if the ejector pin is used, the ejector rod will often leave deep or shallow marks on the plastic parts. If these traces are too deep, the so-called top white phenomenon will appear. In serious cases, the so-called top explosion will occur when the plastic parts are pushed through.


The main reason for the whiteness of plastic parts is that the product has a large mold adhesion force, and the ejection part on the plastic parts causes white marks at the ejection part of the ejector rod. The specific reasons and improvement methods are as follows:


1. Back mold temperature is too low or too high: adjust the appropriate mold temperature.


2. Too fast ejection speed: slow down the ejection speed.


3. With demoulding chamfer: overhaul the mold (polishing).


4. The ejection of finished products is unbalanced (the ejection leaf spring is broken): repair the mold (make the ejection balanced).


5. Insufficient number of thimbles or improper position: increase the number of thimbles or change the position of thimbles.


6. Vacuum occurs in the mold during demoulding: clean the dirt in the ejector pin hole to improve the air inlet effect.


7. The finished bone and column positions are rough (inverted): polish each bone and column position.


8. High injection pressure or holding pressure: reduce the pressure appropriately.


9. The demoulding angle of the finished mold is too small: increase the demoulding angle of the rear mold.


10. Improper action time or position of side slider: repair the mold (make the core pulling action normal).


11. Ejection area is too small or ejection speed is too fast: increase the ejection area or slow down the ejection speed.


12. The injection speed of the last section is too fast (Burr): slow down the injection speed of the next section.


These are the reasons and solutions for the whitening of injection molded products.

Copyright: Shenzhen Zhongyuan Plastic Co., Ltd. | mold processing customized manufacturer. If you want to know the processing price of the factory, how much is it, and which is good, please contact us Yue ICP Bei No. 17060480
鲸鱼体育app下载安卓版本安装| 看球体育直播app官网| 咪咕app下载官方下载| 免费NBA体育直播app| 足球情报哪个网最好| 咪咕app下载官方下载| 极速体育吧NBA直播| 东方赢家app下载| 篮球官方直播| 免费足球直播app软件| 雨燕体育直播| 178足球免费直播| 今晚足球比赛赛事| u球体育app官方下载| 鲸鱼体育app下载安卓版本安装| 下载竞彩足球彩票app| jrs低调看球免费nba高清直播| nba直播(jrs无插件)极速体育| 极速体育jrs直播软件| 五楼直播体育下载| 免费高清篮球直播吧| JRS低调看球免费高清视频直播| 新足球直播手机版| 实况足球网易版官网最新版本| 咪咕篮球赛现场直播| 01体育赛事免费直播| 球赛直播app哪个最全| u球体育app官方下载| 雨燕体育直播| 免费看球直播软件| 足球数据最全的app| 人人体育怎么下载不了| 十大免费体育直播软件| 极速体育jrs直播软件| 178体育苹果下载| 178直播体育在线| 手机足球直播app| cctv5直播在线观看足球直播| 咪咕视频下载免费安装| 看足球比赛哪个app好| 咪咕视频体育直播(无插件)|